Please note: Due to maintenance the shop will be unavailable on Tuesday, November 30, from 06:00 AM until 08:00 AM (CEST)

LF5HTI  581409.322

optical glass klein 4zu3.jpg
Characteristics
nd 1.58144 νd 40.89
ne 1.58482 νe 40.61
nF-nC 0.014220 nF'-nC' 0.014400
Characteristics λ [nm]
n2,325.4 2,325.4 1.54970
n1,970.1 1,970.1 1.55448
n1,529.6 1,529.6 1.55978
n1,060.0 1,060.0 1.56596
nt 1,014.0 1.56674
ns 852.1 1.57015
nr 706.5 1.57490
nC 656.3 1.57724
nC' 643.8 1.57790
Characteristics λ [nm]
n632.8 632.8 1.57852
nD 589.3 1.58132
nd 587.6 1.58144
ne 546.1 1.58482
nF 486.1 1.59145
nF' 480.0 1.59230
ng 435.8 1.59963
nh 404.7 1.60665
ni 365.0 1.61921
Characteristics λ [nm]
n334.1 334.1
n312.6 312.6
n296.7 296.7
n280.4 280.4
n248.3 248.3
Characteristics λ [nm]
τ25/2500 2,500 0.532
τ25/2325 2,325 0.628
τ25/1970 1,970 0.852
τ25/1530 1,530 0.991
τ25/1060 1,060 0.999
τ25/700 700 0.999
τ25/660 660 0.999
τ25/620 620 0.999
τ25/580 580 0.999
τ25/546 546 0.999
τ25/500 500 0.998
τ25/460 460 0.998
τ25/436 436 0.998
τ25/420 420 0.997
τ25/405 405 0.997
τ25/400 400 0.997
τ25/390 390 0.996
τ25/380 380 0.995
τ25/370 370 0.993
τ25/365 365 0.991
τ25/350 350 0.962
τ25/334 334 0.750
τ25/320 320 0.089
τ25/310 310 0.000
τ25/300 300
τ25/290 290
τ25/280 280
τ25/270 270
τ25/260 260
τ25/250 250
Characteristics λ [nm]
τ10/2500 2,500 0.777
τ10/2325 2,325 0.830
τ10/1970 1,970 0.938
τ10/1530 1,530 0.996
τ10/1060 1,060 0.999
τ10/700 700 0.999
τ10/660 660 0.999
τ10/620 620 0.999
τ10/580 580 0.999
τ10/546 546 0.999
τ10/500 500 0.999
τ10/460 460 0.999
τ10/436 436 0.999
τ10/420 420 0.999
τ10/405 405 0.999
τ10/400 400 0.999
τ10/390 390 0.999
τ10/380 380 0.998
τ10/370 370 0.997
τ10/365 365 0.996
τ10/350 350 0.985
τ10/334 334 0.891
τ10/320 320 0.380
τ10/310 310 0.020
τ10/300 300 0.000
τ10/290 290
τ10/280 280
τ10/270 270
τ10/260 260
τ10/250 250
Characteristics
Ps,t 0.2401
PC,s 0.4982
Pd,C 0.2959
Pe,d 0.2373
Pg,F 0.5746
Pi,h 0.8831
P's,t 0.2371
P'C',s 0.5380
P'd,C' 0.2462
P'e,d 0.2343
P'g,F' 0.5090
P'i,h 0.8721
Characteristics
ΔPC,t -0.0006
ΔPC,s 0.0000
ΔPF,e -0.0001
ΔPg,F -0.0004
ΔPi,g -0.0041