BG20

- SCHOTT
- BG20 - BG20
- Thickness
- 1.0
- Reflection factor
- 0.9110
λ [nm] | |
---|---|
200 | < 10⁻³ |
210 | < 10⁻³ |
220 | < 10⁻³ |
230 | < 10⁻³ |
240 | < 10⁻³ |
250 | < 10⁻³ |
260 | 0.040 |
270 | 0.135 |
280 | 0.230 |
290 | 0.355 |
300 | 0.480 |
310 | 0.547 |
320 | 0.660 |
330 | 0.700 |
340 | 0.807 |
350 | 0.420 |
360 | 0.509 |
370 | 0.901 |
380 | 0.990 |
390 | 0.990 |
400 | 0.980 |
410 | 0.995 |
420 | 0.990 |
430 | 0.835 |
440 | 0.701 |
450 | 0.768 |
460 | 0.795 |
470 | 0.733 |
480 | 0.692 |
490 | 0.836 |
λ [nm] | |
---|---|
500 | 0.889 |
510 | 0.763 |
520 | 0.770 |
530 | 0.570 |
540 | 0.797 |
550 | 0.970 |
560 | 0.762 |
570 | 0.244 |
580 | 0.153 |
590 | 0.150 |
600 | 0.580 |
610 | 0.780 |
620 | 0.980 |
630 | 0.978 |
640 | 0.990 |
650 | 1.000 |
660 | 1.000 |
670 | 0.970 |
680 | 0.930 |
690 | 0.930 |
700 | 0.990 |
710 | 0.990 |
720 | 0.980 |
730 | 0.830 |
740 | 0.320 |
750 | 0.393 |
760 | 0.710 |
770 | 0.900 |
780 | 0.870 |
790 | 0.590 |
λ [nm] | |
---|---|
800 | 0.330 |
810 | 0.357 |
820 | 0.710 |
830 | 0.845 |
840 | 0.980 |
850 | 0.960 |
860 | 0.920 |
870 | 0.770 |
880 | 0.620 |
890 | 0.770 |
900 | 0.920 |
910 | 0.937 |
920 | 0.955 |
930 | 0.972 |
940 | 0.990 |
950 | 0.988 |
960 | 0.987 |
970 | 0.985 |
980 | 0.983 |
990 | 0.982 |
1,000 | 0.980 |
1,010 | 0.982 |
1,020 | 0.983 |
1,030 | 0.985 |
1,040 | 0.987 |
1,050 | 0.988 |
1,060 | 0.990 |
1,070 | 0.993 |
1,080 | 0.995 |
1,090 | 0.997 |
λ [nm] | |
---|---|
1,100 | 1.000 |
1,110 | 1.000 |
1,120 | 1.000 |
1,130 | 1.000 |
1,140 | 1.000 |
1,150 | 1.000 |
1,160 | 1.000 |
1,170 | 1.000 |
1,180 | 1.000 |
1,190 | 0.996 |
1,200 | 0.992 |
1,250 | 0.990 |
1,300 | 0.990 |
1,350 | 0.905 |
1,400 | 0.820 |
1,450 | 0.735 |
1,500 | 0.650 |
1,550 | 0.765 |
1,600 | 0.880 |
1,650 | 0.920 |
1,700 | 0.960 |
1,750 | 0.915 |
1,800 | 0.870 |
1,850 | 0.800 |
1,900 | 0.730 |
1,950 | 0.783 |
2,000 | 0.837 |
2,050 | 0.890 |
2,100 | 0.907 |
2,150 | 0.923 |
λ [nm] | |
---|---|
2,200 | 0.940 |
2,250 | 0.915 |
2,300 | 0.890 |
2,350 | 0.875 |
2,400 | 0.860 |
2,450 | 0.845 |
2,500 | 0.830 |
2,550 | 0.855 |
2,600 | 0.880 |
2,650 | 0.905 |
2,700 | 0.930 |
2,750 | 0.760 |
2,800 | 0.590 |
2,850 | 0.598 |
2,900 | 0.605 |
2,950 | 0.613 |
3,000 | 0.620 |
3,050 | 0.623 |
3,100 | 0.625 |
3,150 | 0.627 |
3,200 | 0.630 |
3,250 | 0.615 |
3,300 | 0.600 |
3,350 | 0.585 |
3,400 | 0.570 |
3,450 | 0.542 |
3,500 | 0.513 |
3,550 | 0.485 |
3,600 | 0.457 |
3,650 | 0.428 |
λ [nm] | |
---|---|
3,700 | 0.400 |
3,750 | 0.412 |
3,800 | 0.425 |
3,850 | 0.438 |
3,900 | 0.450 |
3,950 | 0.432 |
4,000 | 0.413 |
4,050 | 0.395 |
4,100 | 0.377 |
4,150 | 0.358 |
4,200 | 0.340 |
4,250 | 0.300 |
4,300 | 0.260 |
4,350 | 0.220 |
4,400 | 0.180 |
4,450 | 0.147 |
4,500 | 0.115 |
4,550 | 0.083 |
4,600 | 0.050 |
4,650 | 0.040 |
4,700 | 0.030 |
4,750 | 0.020 |
4,800 | 0.010 |
4,850 | 0.008 |
4,900 | 0.005 |
4,950 | 0.003 |
5,000 | < 10⁻³ |
5,050 | < 10⁻³ |
5,100 | < 10⁻³ |
5,150 | < 10⁻³ |
Reflection factor | |
---|---|
Pd | 0.911 |
Reference thickness | |
---|---|
d [mm] | 1 |
Refractive Indices n |
---|
nd (587.6 nm) = 1.550 |
Colorimetric evaluation
Illuminant | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
Illuminant | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
Illuminant | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
Density | |
---|---|
p [g/cm3] | 2.86 |
Bubble content | |
---|---|
Bubble class |
Transformation temperature | |
---|---|
Tg [°C] | 561 |
Temperature coefficient | |
---|---|
Tk [nm/°C] |
Chemical Resistance | |
---|---|
FR class | |
SR class | 1.0 |
AR class | 1.0 |
Thermal expansion | |
---|---|
α-30°C/+70°C [10-6/K] | 8.3 |
α20°C/300°C [10-6/K] | 9.3 |
α20°C/200°C [10-6/K] |