BG62HT

Spectral values guaranteed | |
---|---|
τi (405nm) | ≥0.8 |
τi (514nm) | ≥0.9 |
τi (633nm) | ≥0.08 |
τi (694nm) | ≤0.004 |
τi (1060nm) | ≤0.0005 |
- SCHOTT
- BG62HT - BG62HT
- Thickness
- 1.0
- Reflection factor
- 0.9140
λ [nm] | |
---|---|
200 | |
210 | |
220 | |
230 | |
240 | |
250 | |
260 | |
270 | |
280 | |
290 | |
300 | |
310 | < 10⁻³ |
320 | < 10⁻³ |
330 | 0.006 |
340 | 0.095 |
350 | 0.304 |
360 | 0.509 |
370 | 0.642 |
380 | 0.721 |
390 | 0.769 |
400 | 0.802 |
410 | 0.826 |
420 | 0.846 |
430 | 0.863 |
440 | 0.878 |
450 | 0.892 |
460 | 0.904 |
470 | 0.912 |
480 | 0.919 |
490 | 0.925 |
λ [nm] | |
---|---|
500 | 0.926 |
510 | 0.921 |
520 | 0.909 |
530 | 0.886 |
540 | 0.848 |
550 | 0.794 |
560 | 0.723 |
570 | 0.636 |
580 | 0.537 |
590 | 0.434 |
600 | 0.334 |
610 | 0.243 |
620 | 0.168 |
630 | 0.111 |
640 | 0.069 |
650 | 0.041 |
660 | 0.023 |
670 | 0.013 |
680 | 0.007 |
690 | 0.003 |
700 | 0.002 |
710 | < 10⁻³ |
720 | < 10⁻³ |
730 | < 10⁻³ |
740 | < 10⁻³ |
750 | < 10⁻³ |
760 | < 10⁻³ |
770 | < 10⁻³ |
780 | < 10⁻³ |
790 | < 10⁻³ |
λ [nm] | |
---|---|
800 | < 10⁻³ |
810 | < 10⁻³ |
820 | < 10⁻³ |
830 | < 10⁻³ |
840 | < 10⁻³ |
850 | < 10⁻³ |
860 | < 10⁻³ |
870 | < 10⁻³ |
880 | < 10⁻³ |
890 | < 10⁻³ |
900 | < 10⁻³ |
910 | < 10⁻³ |
920 | < 10⁻³ |
930 | < 10⁻³ |
940 | < 10⁻³ |
950 | < 10⁻³ |
960 | < 10⁻³ |
970 | < 10⁻³ |
980 | < 10⁻³ |
990 | < 10⁻³ |
1,000 | < 10⁻³ |
1,010 | < 10⁻³ |
1,020 | < 10⁻³ |
1,030 | < 10⁻³ |
1,040 | < 10⁻³ |
1,050 | < 10⁻³ |
1,060 | < 10⁻³ |
1,070 | < 10⁻³ |
1,080 | < 10⁻³ |
1,090 | < 10⁻³ |
λ [nm] | |
---|---|
1,100 | < 10⁻³ |
1,110 | < 10⁻³ |
1,120 | 0.001 |
1,130 | 0.001 |
1,140 | 0.002 |
1,150 | 0.002 |
1,160 | 0.003 |
1,170 | 0.003 |
1,180 | 0.004 |
1,190 | 0.005 |
1,200 | 0.006 |
1,250 | 0.014 |
1,300 | 0.029 |
1,350 | 0.056 |
1,400 | 0.095 |
1,450 | 0.147 |
1,500 | 0.210 |
1,550 | 0.281 |
1,600 | 0.356 |
1,650 | 0.433 |
1,700 | 0.504 |
1,750 | 0.570 |
1,800 | 0.628 |
1,850 | 0.681 |
1,900 | 0.728 |
1,950 | 0.761 |
2,000 | 0.794 |
2,050 | 0.821 |
2,100 | 0.846 |
2,150 | 0.862 |
λ [nm] | |
---|---|
2,200 | 0.876 |
2,250 | 0.886 |
2,300 | 0.901 |
2,350 | 0.908 |
2,400 | 0.914 |
2,450 | 0.921 |
2,500 | 0.920 |
2,550 | 0.921 |
2,600 | 0.921 |
2,650 | 0.920 |
2,700 | 0.917 |
2,750 | 0.906 |
2,800 | 0.863 |
2,850 | 0.785 |
2,900 | 0.712 |
2,950 | 0.655 |
3,000 | 0.607 |
3,050 | 0.564 |
3,100 | 0.522 |
3,150 | 0.483 |
3,200 | 0.448 |
3,250 | 0.417 |
3,300 | 0.392 |
3,350 | 0.371 |
3,400 | 0.356 |
3,450 | 0.346 |
3,500 | 0.342 |
3,550 | 0.345 |
3,600 | 0.352 |
3,650 | 0.366 |
λ [nm] | |
---|---|
3,700 | 0.384 |
3,750 | 0.400 |
3,800 | 0.402 |
3,850 | 0.375 |
3,900 | 0.330 |
3,950 | 0.278 |
4,000 | 0.215 |
4,050 | 0.139 |
4,100 | 0.078 |
4,150 | 0.042 |
4,200 | 0.023 |
4,250 | 0.015 |
4,300 | 0.014 |
4,350 | 0.014 |
4,400 | 0.013 |
4,450 | 0.011 |
4,500 | 0.008 |
4,550 | 0.007 |
4,600 | 0.007 |
4,650 | 0.009 |
4,700 | 0.014 |
4,750 | 0.022 |
4,800 | 0.034 |
4,850 | 0.047 |
4,900 | 0.063 |
4,950 | 0.085 |
5,000 | 0.110 |
5,050 | 0.133 |
5,100 | 0.151 |
5,150 | 0.158 |
Reflection factor | |
---|---|
Pd | 0.914 |
Reference thickness | |
---|---|
d [mm] | 1 |
Spectral values guaranteed | |
---|---|
τi (405nm) | ≥0.8 |
τi (514nm) | ≥0.9 |
τi (633nm) | ≥0.08 |
τi (694nm) | ≤0.004 |
τi (1060nm) | ≤0.0005 |
Refractive Indices n |
---|
nF (486.1 nm) = 1.546 |
nh (404.7 nm) = 1.554 |
ng (435.8 nm) = 1.550 |
ns (852.1 nm) = 1.533 |
ne (546.1 nm) = 1.542 |
nd (587.6 nm) = 1.540 |
Colorimetric evaluation
Illuminant | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.317 | 0.252 | 0.215 |
y | 0.438 | 0.438 | 0.430 |
Y | 52 | 37 | 28 |
λd [nm] | 499 | 497 | 496 |
Pe | 0.30 | 0.45 | 0.54 |
Illuminant | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.298 | 0.238 | 0.205 |
y | 0.418 | 0.413 | 0.403 |
Y | 54 | 39 | 30 |
λd [nm] | 497 | 496 | 495 |
Pe | 0.31 | 0.46 | 0.55 |
Illuminant | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.226 | 0.191 | 0.172 |
y | 0.314 | 0.299 | 0.288 |
Y | 61 | 47 | 38 |
λd [nm] | 489 | 489 | 488 |
Pe | 0.33 | 0.47 | 0.55 |
Density | |
---|---|
p [g/cm3] | 2.848 |
Bubble content | |
---|---|
Bubble class |
Transformation temperature | |
---|---|
Tg [°C] | 410 |
Temperature coefficient | |
---|---|
Tk [nm/°C] |
Chemical Resistance | |
---|---|
FR class | 1 |
SR class | 52.3 |
AR class | 3.3 |
Thermal expansion | |
---|---|
α-30°C/+70°C [10-6/K] | 11.79 |
α20°C/300°C [10-6/K] | 13.65 |
α20°C/200°C [10-6/K] |