玻璃类型 |
物品编号 |
长度 |
宽度 |
厚度 |
重量 |
---|
BG39
- SCHOTT
- BG39 - BG39
- 厚度
- 1.0
- 反射系数
- 0.9144
λ [nm] | |
---|---|
200 | < 10⁻³ |
210 | < 10⁻³ |
220 | < 10⁻³ |
230 | < 10⁻³ |
240 | < 10⁻³ |
250 | < 10⁻³ |
260 | < 10⁻³ |
270 | < 10⁻³ |
280 | < 10⁻³ |
290 | < 10⁻³ |
300 | < 10⁻³ |
310 | < 10⁻³ |
320 | 0.042 |
330 | 0.256 |
340 | 0.494 |
350 | 0.647 |
360 | 0.732 |
370 | 0.783 |
380 | 0.818 |
390 | 0.845 |
400 | 0.867 |
410 | 0.886 |
420 | 0.902 |
430 | 0.917 |
440 | 0.929 |
450 | 0.939 |
460 | 0.948 |
470 | 0.956 |
480 | 0.963 |
490 | 0.967 |
λ [nm] | |
---|---|
500 | 0.970 |
510 | 0.970 |
520 | 0.967 |
530 | 0.957 |
540 | 0.941 |
550 | 0.914 |
560 | 0.874 |
570 | 0.820 |
580 | 0.751 |
590 | 0.668 |
600 | 0.575 |
610 | 0.476 |
620 | 0.378 |
630 | 0.287 |
640 | 0.207 |
650 | 0.142 |
660 | 0.092 |
670 | 0.057 |
680 | 0.034 |
690 | 0.019 |
700 | 0.010 |
710 | 0.005 |
720 | 0.003 |
730 | 0.001 |
740 | < 10⁻³ |
750 | < 10⁻³ |
760 | < 10⁻³ |
770 | < 10⁻³ |
780 | < 10⁻³ |
790 | < 10⁻³ |
λ [nm] | |
---|---|
800 | < 10⁻³ |
810 | < 10⁻³ |
820 | < 10⁻³ |
830 | < 10⁻³ |
840 | < 10⁻³ |
850 | < 10⁻³ |
860 | < 10⁻³ |
870 | < 10⁻³ |
880 | < 10⁻³ |
890 | < 10⁻³ |
900 | < 10⁻³ |
910 | < 10⁻³ |
920 | < 10⁻³ |
930 | < 10⁻³ |
940 | < 10⁻³ |
950 | < 10⁻³ |
960 | < 10⁻³ |
970 | < 10⁻³ |
980 | < 10⁻³ |
990 | < 10⁻³ |
1,000 | < 10⁻³ |
1,010 | < 10⁻³ |
1,020 | < 10⁻³ |
1,030 | < 10⁻³ |
1,040 | < 10⁻³ |
1,050 | < 10⁻³ |
1,060 | < 10⁻³ |
1,070 | < 10⁻³ |
1,080 | < 10⁻³ |
1,090 | < 10⁻³ |
λ [nm] | |
---|---|
1,100 | < 10⁻³ |
1,110 | < 10⁻³ |
1,120 | < 10⁻³ |
1,130 | < 10⁻³ |
1,140 | < 10⁻³ |
1,150 | 0.001 |
1,160 | 0.001 |
1,170 | 0.002 |
1,180 | 0.002 |
1,190 | 0.002 |
1,200 | 0.003 |
1,250 | 0.007 |
1,300 | 0.020 |
1,350 | 0.038 |
1,400 | 0.070 |
1,450 | 0.121 |
1,500 | 0.184 |
1,550 | 0.262 |
1,600 | 0.344 |
1,650 | 0.431 |
1,700 | 0.510 |
1,750 | 0.586 |
1,800 | 0.646 |
1,850 | 0.697 |
1,900 | 0.740 |
1,950 | 0.783 |
2,000 | 0.810 |
2,050 | 0.836 |
2,100 | 0.856 |
2,150 | 0.869 |
λ [nm] | |
---|---|
2,200 | 0.866 |
2,250 | 0.859 |
2,300 | 0.860 |
2,350 | 0.860 |
2,400 | 0.860 |
2,450 | 0.853 |
2,500 | 0.820 |
2,550 | 0.758 |
2,600 | 0.740 |
2,650 | 0.714 |
2,700 | 0.690 |
2,750 | 0.592 |
2,800 | 0.330 |
2,850 | 0.136 |
2,900 | 0.070 |
2,950 | 0.036 |
3,000 | 0.020 |
3,050 | 0.011 |
3,100 | 0.006 |
3,150 | 0.003 |
3,200 | 0.002 |
3,250 | < 10⁻³ |
3,300 | < 10⁻³ |
3,350 | < 10⁻³ |
3,400 | < 10⁻³ |
3,450 | < 10⁻³ |
3,500 | < 10⁻³ |
3,550 | < 10⁻³ |
3,600 | < 10⁻³ |
3,650 | < 10⁻³ |
λ [nm] | |
---|---|
3,700 | 0.001 |
3,750 | 0.002 |
3,800 | 0.002 |
3,850 | 0.002 |
3,900 | 0.002 |
3,950 | 0.001 |
4,000 | < 10⁻³ |
4,050 | < 10⁻³ |
4,100 | < 10⁻³ |
4,150 | < 10⁻³ |
4,200 | < 10⁻³ |
4,250 | < 10⁻³ |
4,300 | < 10⁻³ |
4,350 | < 10⁻³ |
4,400 | < 10⁻³ |
4,450 | < 10⁻³ |
4,500 | < 10⁻³ |
4,550 | < 10⁻³ |
4,600 | < 10⁻³ |
4,650 | 0.001 |
4,700 | 0.002 |
4,750 | 0.002 |
4,800 | 0.003 |
4,850 | 0.003 |
4,900 | 0.003 |
4,950 | 0.003 |
5,000 | 0.003 |
5,050 | 0.003 |
5,100 | 0.004 |
5,150 | 0.004 |
反射系数 | |
---|---|
Pd | 0.914 |
参考厚度 | |
---|---|
d [mm] | 1 |
承诺光谱值 | |
---|---|
τi (350nm) | ≥0.6 |
τi (405nm) | ≥0.85 |
τi (514nm) | ≥0.93 |
τi (633nm) | ≤0.3 |
τi (694nm) | ≤0.03 |
τi (1060nm) | ≤0.001 |
折射率 n |
---|
nF (486.1 nm) = 1.542 |
nh (404.7 nm) = 1.551 |
ng (435.8 nm) = 1.547 |
ns (852.1 nm) = 1.529 |
ne (546.1 nm) = 1.538 |
nd (587.6 nm) = 1.536 |
色度评估
光源 | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.365 | 0.314 | 0.279 |
y | 0.434 | 0.445 | 0.450 |
Y | 66 | 53 | 45 |
λd [nm] | 500 | 500 | 499 |
Pe | 0.19 | 0.31 | 0.39 |
光源 | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.344 | 0.296 | 0.264 |
y | 0.419 | 0.425 | 0.427 |
Y | 67 | 55 | 47 |
λd [nm] | 498 | 498 | 497 |
Pe | 0.19 | 0.31 | 0.39 |
光源 | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.257 | 0.226 | 0.207 |
y | 0.326 | 0.322 | 0.318 |
Y | 73 | 62 | 55 |
λd [nm] | 491 | 490 | 490 |
Pe | 0.21 | 0.32 | 0.39 |
密度 | |
---|---|
p [g/cm3] | 2.74 |
气泡含量 | |
---|---|
气泡等级 | 2 |
玻转温度 | |
---|---|
Tg [°C] | 322 |
温度系数 | |
---|---|
Tk [nm/°C] |
耐化学性 | |
---|---|
耐污性 | 0 |
耐酸性 | 5.1 |
耐碱性 | 3.0 |
热膨胀 | |
---|---|
α-30°C/+70°C [10-6/K] | 11.6 |
α20°C/300°C [10-6/K] | |
α20°C/200°C [10-6/K] | 13.1 |