技术规格
折射率
| 特性 | λ [nm] | |
|---|---|---|
| n2,325.4 | 2,325.4 | 1.46180 |
| n1,970.1 | 1,970.1 | 1.46738 |
| n1,529.6 | 1,529.6 | 1.47312 |
| n1,060.0 | 1,060.0 | 1.47855 |
| nt | 1,014.0 | 1.47912 |
| ns | 852.1 | 1.48137 |
| nr | 706.5 | 1.48409 |
| nC | 656.3 | 1.48534 |
| nC' | 643.8 | 1.48568 |
| 特性 | λ [nm] | |
|---|---|---|
| n632.8 | 632.8 | 1.48600 |
| nD | 589.3 | 1.48742 |
| nd | 587.6 | 1.48748 |
| ne | 546.1 | 1.48913 |
| nF | 486.1 | 1.49225 |
| nF' | 480.0 | 1.49264 |
| ng | 435.8 | 1.49591 |
| nh | 404.7 | 1.49892 |
| ni | 365.0 | 1.50398 |
| 特性 | λ [nm] | |
|---|---|---|
| n334.1 | 334.1 | 1.50935 |
| n312.6 | 312.6 | 1.51423 |
| n296.7 | 296.7 | 1.51861 |
| n280.4 | 280.4 | 1.52409 |
| n248.3 | 248.3 | |
内部透射率
| 特性 | λ [nm] | |
|---|---|---|
| τ25/2500 | 2,500 | 0.385 |
| τ25/2325 | 2,325 | 0.628 |
| τ25/1970 | 1,970 | 0.930 |
| τ25/1530 | 1,530 | 0.965 |
| τ25/1060 | 1,060 | 0.998 |
| τ25/700 | 700 | 0.997 |
| τ25/660 | 660 | 0.995 |
| τ25/620 | 620 | 0.994 |
| τ25/580 | 580 | 0.995 |
| τ25/546 | 546 | 0.995 |
| τ25/500 | 500 | 0.994 |
| τ25/460 | 460 | 0.995 |
| τ25/436 | 436 | 0.996 |
| τ25/420 | 420 | 0.997 |
| τ25/405 | 405 | 0.997 |
| τ25/400 | 400 | 0.997 |
| τ25/390 | 390 | 0.997 |
| τ25/380 | 380 | 0.996 |
| τ25/370 | 370 | 0.996 |
| τ25/365 | 365 | 0.996 |
| τ25/350 | 350 | 0.994 |
| τ25/334 | 334 | 0.989 |
| τ25/320 | 320 | 0.979 |
| τ25/310 | 310 | 0.958 |
| τ25/300 | 300 | 0.900 |
| τ25/290 | 290 | 0.760 |
| τ25/280 | 280 | 0.510 |
| τ25/270 | 270 | 0.220 |
| τ25/260 | 260 | 0.050 |
| τ25/250 | 250 | 0.002 |
| 特性 | λ [nm] | |
|---|---|---|
| τ10/2500 | 2,500 | 0.683 |
| τ10/2325 | 2,325 | 0.830 |
| τ10/1970 | 1,970 | 0.971 |
| τ10/1530 | 1,530 | 0.986 |
| τ10/1060 | 1,060 | 0.999 |
| τ10/700 | 700 | 0.999 |
| τ10/660 | 660 | 0.998 |
| τ10/620 | 620 | 0.998 |
| τ10/580 | 580 | 0.998 |
| τ10/546 | 546 | 0.998 |
| τ10/500 | 500 | 0.998 |
| τ10/460 | 460 | 0.998 |
| τ10/436 | 436 | 0.998 |
| τ10/420 | 420 | 0.999 |
| τ10/405 | 405 | 0.999 |
| τ10/400 | 400 | 0.999 |
| τ10/390 | 390 | 0.999 |
| τ10/380 | 380 | 0.998 |
| τ10/370 | 370 | 0.999 |
| τ10/365 | 365 | 0.998 |
| τ10/350 | 350 | 0.998 |
| τ10/334 | 334 | 0.996 |
| τ10/320 | 320 | 0.992 |
| τ10/310 | 310 | 0.983 |
| τ10/300 | 300 | 0.959 |
| τ10/290 | 290 | 0.896 |
| τ10/280 | 280 | 0.764 |
| τ10/270 | 270 | 0.546 |
| τ10/260 | 260 | 0.302 |
| τ10/250 | 250 | 0.120 |
部分色散
| 特性 | |
|---|---|
| Ps,t | 0.3253 |
| PC,s | 0.5742 |
| Pd,C | 0.3098 |
| Pe,d | 0.2388 |
| Pg,F | 0.5288 |
| Pi,h | 0.7315 |
| P's,t | 0.3234 |
| P'C',s | 0.6203 |
| P'd,C' | 0.2584 |
| P'e,d | 0.2374 |
| P'g,F' | 0.4703 |
| P'i,h | 0.7271 |
| 特性 | |
|---|---|
| ΔPC,t | 0.0202 |
| ΔPC,s | 0.0070 |
| ΔPF,e | 0.0001 |
| ΔPg,F | 0.0036 |
| ΔPi,g | 0.0321 |
下载
TIE's - 技术信息
TIE-19: Temperature Coefficient of the Refractive Index (US)
PDF
450 kB
TIE-25: Striae in Optical Glass (US)
PDF
1.24 MB
TIE-27: Stress in Optical Glass (US)
PDF
710 kB
TIE-28: Bubbles and Inclusions in Optical Glass (US)
PDF
260 kB
TIE-29: Refractive Index and Dispersion (US)
PDF
1 MB
TIE-30: Chemical Properties of Optical Glass (US)
PDF
210 kB
TIE-31: Mechanical and Thermal Properties of Optical Glass (US)
PDF
220 kB
TIE-32: Thermal Loads on Optical Glass (US)
PDF
140 kB
TIE-33: Bending Strength of Optical Glass and ZERODUR® (US)
PDF
2.75 MB
TIE-35: Transmittance of Optical Glass (US)
PDF
500 kB
TIE-36: Fluorescence of Optical Glass (US)
PDF
1.02 MB
TIE-40: Optical Glass for Precision Molding (US)
PDF
610 kB
TIE-41: Large Optical Glass Blanks (US)
PDF
2.06 MB