技术规格
折射率
| 特性 | λ [nm] | |
|---|---|---|
| n2,325.4 | 2,325.4 | 1.55583 |
| n1,970.1 | 1,970.1 | 1.56169 |
| n1,529.6 | 1,529.6 | 1.56784 |
| n1,060.0 | 1,060.0 | 1.57407 |
| nt | 1,014.0 | 1.57476 |
| ns | 852.1 | 1.57762 |
| nr | 706.5 | 1.58127 |
| nC | 656.3 | 1.58299 |
| nC' | 643.8 | 1.58347 |
| 特性 | λ [nm] | |
|---|---|---|
| n632.8 | 632.8 | 1.58392 |
| nD | 589.3 | 1.58591 |
| nd | 587.6 | 1.58600 |
| ne | 546.1 | 1.58835 |
| nF | 486.1 | 1.59284 |
| nF' | 480.0 | 1.59340 |
| ng | 435.8 | 1.59817 |
| nh | 404.7 | 1.60260 |
| ni | 365.0 | 1.61013 |
| 特性 | λ [nm] | |
|---|---|---|
| n334.1 | 334.1 | 1.61826 |
| n312.6 | 312.6 | |
| n296.7 | 296.7 | |
| n280.4 | 280.4 | |
| n248.3 | 248.3 | |
内部透射率
| 特性 | λ [nm] | |
|---|---|---|
| τ25/2500 | 2,500 | 0.400 |
| τ25/2325 | 2,325 | 0.630 |
| τ25/1970 | 1,970 | 0.890 |
| τ25/1530 | 1,530 | 0.978 |
| τ25/1060 | 1,060 | 0.997 |
| τ25/700 | 700 | 0.997 |
| τ25/660 | 660 | 0.997 |
| τ25/620 | 620 | 0.997 |
| τ25/580 | 580 | 0.997 |
| τ25/546 | 546 | 0.997 |
| τ25/500 | 500 | 0.995 |
| τ25/460 | 460 | 0.991 |
| τ25/436 | 436 | 0.989 |
| τ25/420 | 420 | 0.987 |
| τ25/405 | 405 | 0.985 |
| τ25/400 | 400 | 0.984 |
| τ25/390 | 390 | 0.980 |
| τ25/380 | 380 | 0.973 |
| τ25/370 | 370 | 0.960 |
| τ25/365 | 365 | 0.950 |
| τ25/350 | 350 | 0.870 |
| τ25/334 | 334 | 0.610 |
| τ25/320 | 320 | 0.160 |
| τ25/310 | 310 | 0.000 |
| τ25/300 | 300 | |
| τ25/290 | 290 | |
| τ25/280 | 280 | |
| τ25/270 | 270 | |
| τ25/260 | 260 | |
| τ25/250 | 250 | |
| 特性 | λ [nm] | |
|---|---|---|
| τ10/2500 | 2,500 | 0.693 |
| τ10/2325 | 2,325 | 0.831 |
| τ10/1970 | 1,970 | 0.954 |
| τ10/1530 | 1,530 | 0.991 |
| τ10/1060 | 1,060 | 0.999 |
| τ10/700 | 700 | 0.999 |
| τ10/660 | 660 | 0.999 |
| τ10/620 | 620 | 0.999 |
| τ10/580 | 580 | 0.999 |
| τ10/546 | 546 | 0.999 |
| τ10/500 | 500 | 0.998 |
| τ10/460 | 460 | 0.996 |
| τ10/436 | 436 | 0.996 |
| τ10/420 | 420 | 0.995 |
| τ10/405 | 405 | 0.994 |
| τ10/400 | 400 | 0.994 |
| τ10/390 | 390 | 0.992 |
| τ10/380 | 380 | 0.989 |
| τ10/370 | 370 | 0.984 |
| τ10/365 | 365 | 0.980 |
| τ10/350 | 350 | 0.946 |
| τ10/334 | 334 | 0.821 |
| τ10/320 | 320 | 0.480 |
| τ10/310 | 310 | 0.123 |
| τ10/300 | 300 | 0.000 |
| τ10/290 | 290 | |
| τ10/280 | 280 | |
| τ10/270 | 270 | |
| τ10/260 | 260 | |
| τ10/250 | 250 | |
部分色散
| 特性 | |
|---|---|
| Ps,t | 0.2903 |
| PC,s | 0.5454 |
| Pd,C | 0.3052 |
| Pe,d | 0.2385 |
| Pg,F | 0.5414 |
| Pi,h | 0.7652 |
| P's,t | 0.2880 |
| P'C',s | 0.5894 |
| P'd,C' | 0.2545 |
| P'e,d | 0.2366 |
| P'g,F' | 0.4807 |
| P'i,h | 0.7590 |
| 特性 | |
|---|---|
| ΔPC,t | 0.0085 |
| ΔPC,s | 0.0038 |
| ΔPF,e | -0.0008 |
| ΔPg,F | -0.0024 |
| ΔPi,g | -0.0113 |
下载
TIE's - 技术信息
TIE-19: Temperature Coefficient of the Refractive Index (US)
PDF
450 kB
TIE-25: Striae in Optical Glass (US)
PDF
1.24 MB
TIE-27: Stress in Optical Glass (US)
PDF
710 kB
TIE-28: Bubbles and Inclusions in Optical Glass (US)
PDF
260 kB
TIE-29: Refractive Index and Dispersion (US)
PDF
1 MB
TIE-30: Chemical Properties of Optical Glass (US)
PDF
210 kB
TIE-31: Mechanical and Thermal Properties of Optical Glass (US)
PDF
220 kB
TIE-32: Thermal Loads on Optical Glass (US)
PDF
140 kB
TIE-33: Bending Strength of Optical Glass and ZERODUR® (US)
PDF
2.75 MB
TIE-35: Transmittance of Optical Glass (US)
PDF
500 kB
TIE-36: Fluorescence of Optical Glass (US)
PDF
1.02 MB
TIE-40: Optical Glass for Precision Molding (US)
PDF
610 kB
TIE-41: Large Optical Glass Blanks (US)
PDF
2.06 MB