Technical Details
Internal Transmittance (Chart)
- SCHOTT
- S8806A - S8806A
- Thickness
- 2.5
- Reflection factor
- 0.8780
Internal Transmittance (Table)
| λ [nm] | |
|---|---|
| 200 | |
| 210 | |
| 220 | |
| 230 | |
| 240 | |
| 250 | |
| 260 | |
| 270 | |
| 280 | |
| 290 | < 10⁻³ |
| 300 | 0.011 |
| 310 | 0.120 |
| 320 | 0.286 |
| 330 | 0.112 |
| 340 | 0.324 |
| 350 | 0.001 |
| 360 | 0.006 |
| 370 | 0.901 |
| 380 | 0.918 |
| 390 | 0.957 |
| 400 | 0.957 |
| 410 | 0.968 |
| 420 | 0.880 |
| 430 | 0.309 |
| 440 | 0.837 |
| 450 | 0.725 |
| 460 | 0.373 |
| 470 | 0.320 |
| 480 | 0.388 |
| 490 | 0.798 |
| λ [nm] | |
|---|---|
| 500 | 0.376 |
| 510 | 0.027 |
| 520 | 0.026 |
| 530 | 0.011 |
| 540 | 0.454 |
| 550 | 0.805 |
| 560 | 0.693 |
| 570 | 0.002 |
| 580 | |
| 590 | |
| 600 | 0.051 |
| 610 | 0.735 |
| 620 | 0.833 |
| 630 | 0.760 |
| 640 | 0.906 |
| 650 | 0.973 |
| 660 | 0.954 |
| 670 | 0.675 |
| 680 | 0.325 |
| 690 | 0.534 |
| 700 | 0.833 |
| 710 | 0.897 |
| 720 | 0.739 |
| 730 | 0.072 |
| 740 | |
| 750 | |
| 760 | 0.010 |
| 770 | 0.272 |
| 780 | 0.227 |
| 790 | 0.005 |
| λ [nm] | |
|---|---|
| 800 | |
| 810 | |
| 820 | 0.021 |
| 830 | 0.266 |
| 840 | 0.680 |
| 850 | 0.707 |
| 860 | 0.230 |
| 870 | 0.076 |
| 880 | 0.083 |
| 890 | 0.210 |
| 900 | 0.411 |
| 910 | 0.633 |
| 920 | 0.820 |
| 930 | 0.934 |
| 940 | 0.981 |
| 950 | 0.993 |
| 960 | 0.996 |
| 970 | 0.996 |
| 980 | 0.996 |
| 990 | 0.995 |
| 1,000 | 0.995 |
| 1,010 | 0.995 |
| 1,020 | 0.996 |
| 1,030 | 0.996 |
| 1,040 | 0.996 |
| 1,050 | 0.995 |
| 1,060 | 0.993 |
| 1,070 | 0.990 |
| 1,080 | 0.990 |
| 1,090 | 0.993 |
| λ [nm] | |
|---|---|
| 1,100 | 0.996 |
| 1,110 | 0.997 |
| 1,120 | 0.998 |
| 1,130 | 0.999 |
| 1,140 | 0.999 |
| 1,150 | 1.000 |
| 1,160 | 1.000 |
| 1,170 | 0.999 |
| 1,180 | 0.999 |
| 1,190 | 0.997 |
| 1,200 | 0.994 |
| 1,250 | 0.992 |
| 1,300 | 0.996 |
| 1,350 | 0.980 |
| 1,400 | 0.944 |
| 1,450 | 0.923 |
| 1,500 | 0.847 |
| 1,550 | 0.727 |
| 1,600 | 0.678 |
| 1,650 | 0.723 |
| 1,700 | 0.776 |
| 1,750 | 0.862 |
| 1,800 | 0.938 |
| 1,850 | 0.941 |
| 1,900 | 0.925 |
| 1,950 | 0.930 |
| 2,000 | 0.940 |
| 2,050 | 0.943 |
| 2,100 | 0.935 |
| 2,150 | 0.911 |
| λ [nm] | |
|---|---|
| 2,200 | 0.856 |
| 2,250 | 0.693 |
| 2,300 | 0.351 |
| 2,350 | 0.135 |
| 2,400 | 0.079 |
| 2,450 | 0.074 |
| 2,500 | 0.093 |
| 2,550 | 0.117 |
| 2,600 | 0.264 |
| 2,650 | 0.355 |
| 2,700 | 0.438 |
| 2,750 | 0.403 |
| 2,800 | 0.273 |
| 2,850 | 0.233 |
| 2,900 | 0.236 |
| 2,950 | 0.250 |
| 3,000 | 0.263 |
| 3,050 | 0.271 |
| 3,100 | 0.274 |
| 3,150 | 0.268 |
| 3,200 | 0.251 |
| 3,250 | 0.211 |
| 3,300 | 0.141 |
| 3,350 | 0.067 |
| 3,400 | 0.021 |
| 3,450 | 0.004 |
| 3,500 | < 10⁻³ |
| 3,550 | |
| 3,600 | |
| 3,650 | |
| λ [nm] | |
|---|---|
| 3,700 | |
| 3,750 | |
| 3,800 | |
| 3,850 | < 10⁻³ |
| 3,900 | < 10⁻³ |
| 3,950 | < 10⁻³ |
| 4,000 | < 10⁻³ |
| 4,050 | < 10⁻³ |
| 4,100 | < 10⁻³ |
| 4,150 | < 10⁻³ |
| 4,200 | |
| 4,250 | |
| 4,300 | < 10⁻³ |
| 4,350 | < 10⁻³ |
| 4,400 | < 10⁻³ |
| 4,450 | < 10⁻³ |
| 4,500 | < 10⁻³ |
| 4,550 | < 10⁻³ |
| 4,600 | < 10⁻³ |
| 4,650 | < 10⁻³ |
| 4,700 | |
| 4,750 | < 10⁻³ |
| 4,800 | < 10⁻³ |
| 4,850 | < 10⁻³ |
| 4,900 | < 10⁻³ |
| 4,950 | < 10⁻³ |
| 5,000 | < 10⁻³ |
| 5,050 | |
| 5,100 | |
| 5,150 | |
Optical values
| Reflection factor | |
|---|---|
| Pd | 0.878 |
| Reference thickness | |
|---|---|
| d [mm] | 2 |
| Spectral values guaranteed | |
|---|---|
| τi (550nm) | >0.76 |
| Refractive Indices n |
|---|
| nF (486.1 nm) = 1.694 |
| nh (404.7 nm) = 1.707 |
| ng (435.8 nm) = 1.701 |
| ns (852.1 nm) = 1.674 |
| ne (546.1 nm) = 1.688 |
| nd (587.6 nm) = 1.685 |
Colorimetric evaluation
| Illuminant | A(Planck T = 2347K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | |||
| y | |||
| Y | |||
| λd [nm] | |||
| Pe | |||
| Illuminant | Planck T = 3200 K | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | |||
| y | |||
| Y | |||
| λd [nm] | |||
| Pe | |||
| Illuminant | D65 (TC = 6504 K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | |||
| y | |||
| Y | |||
| λd [nm] | |||
| Pe | |||
Physical values
| Density | |
|---|---|
| p [g/cm3] | 3.4874 |
| Bubble content | |
|---|---|
| Bubble class | - |
| Transformation temperature | |
|---|---|
| Tg [°C] | 653 |
| Temperature coefficient | |
|---|---|
| Tk [nm/°C] | |
| Chemical Resistance | |
|---|---|
| FR class | 4 |
| SR class | 52.0 |
| AR class | 1.3 |
| Thermal expansion | |
|---|---|
| α-30°C/+70°C [10-6/K] | 6.13 |
| α20°C/300°C [10-6/K] | 7.27 |
| α20°C/200°C [10-6/K] | |