技术规格
折射率
| 特性 | λ [nm] | |
|---|---|---|
| n2,325.4 | 2,325.4 | 1.71338 |
| n1,970.1 | 1,970.1 | 1.72058 |
| n1,529.6 | 1,529.6 | 1.72830 |
| n1,060.0 | 1,060.0 | 1.73669 |
| nt | 1,014.0 | 1.73770 |
| ns | 852.1 | 1.74198 |
| nr | 706.5 | 1.74775 |
| nC | 656.3 | 1.75054 |
| nC' | 643.8 | 1.75132 |
| 特性 | λ [nm] | |
|---|---|---|
| n632.8 | 632.8 | 1.75206 |
| nD | 589.3 | 1.75535 |
| nd | 587.6 | 1.75550 |
| ne | 546.1 | 1.75944 |
| nF | 486.1 | 1.76708 |
| nF' | 480.0 | 1.76804 |
| ng | 435.8 | 1.77633 |
| nh | 404.7 | 1.78414 |
| ni | 365.0 | |
| 特性 | λ [nm] | |
|---|---|---|
| n334.1 | 334.1 | |
| n312.6 | 312.6 | |
| n296.7 | 296.7 | |
| n280.4 | 280.4 | |
| n248.3 | 248.3 | |
内部透射率
| 特性 | λ [nm] | |
|---|---|---|
| τ25/2500 | 2,500 | 0.232 |
| τ25/2325 | 2,325 | 0.598 |
| τ25/1970 | 1,970 | 0.922 |
| τ25/1530 | 1,530 | 0.991 |
| τ25/1060 | 1,060 | 0.998 |
| τ25/700 | 700 | 0.997 |
| τ25/660 | 660 | 0.995 |
| τ25/620 | 620 | 0.995 |
| τ25/580 | 580 | 0.995 |
| τ25/546 | 546 | 0.995 |
| τ25/500 | 500 | 0.992 |
| τ25/460 | 460 | 0.982 |
| τ25/436 | 436 | 0.973 |
| τ25/420 | 420 | 0.965 |
| τ25/405 | 405 | 0.949 |
| τ25/400 | 400 | 0.941 |
| τ25/390 | 390 | 0.914 |
| τ25/380 | 380 | 0.862 |
| τ25/370 | 370 | 0.775 |
| τ25/365 | 365 | 0.712 |
| τ25/350 | 350 | 0.450 |
| τ25/334 | 334 | 0.145 |
| τ25/320 | 320 | 0.014 |
| τ25/310 | 310 | |
| τ25/300 | 300 | |
| τ25/290 | 290 | |
| τ25/280 | 280 | |
| τ25/270 | 270 | |
| τ25/260 | 260 | |
| τ25/250 | 250 | |
| 特性 | λ [nm] | |
|---|---|---|
| τ10/2500 | 2,500 | 0.558 |
| τ10/2325 | 2,325 | 0.814 |
| τ10/1970 | 1,970 | 0.968 |
| τ10/1530 | 1,530 | 0.997 |
| τ10/1060 | 1,060 | 0.999 |
| τ10/700 | 700 | 0.999 |
| τ10/660 | 660 | 0.998 |
| τ10/620 | 620 | 0.998 |
| τ10/580 | 580 | 0.998 |
| τ10/546 | 546 | 0.998 |
| τ10/500 | 500 | 0.997 |
| τ10/460 | 460 | 0.993 |
| τ10/436 | 436 | 0.989 |
| τ10/420 | 420 | 0.986 |
| τ10/405 | 405 | 0.979 |
| τ10/400 | 400 | 0.976 |
| τ10/390 | 390 | 0.965 |
| τ10/380 | 380 | 0.943 |
| τ10/370 | 370 | 0.903 |
| τ10/365 | 365 | 0.873 |
| τ10/350 | 350 | 0.727 |
| τ10/334 | 334 | 0.462 |
| τ10/320 | 320 | 0.181 |
| τ10/310 | 310 | 0.040 |
| τ10/300 | 300 | |
| τ10/290 | 290 | |
| τ10/280 | 280 | |
| τ10/270 | 270 | |
| τ10/260 | 260 | |
| τ10/250 | 250 | |
部分色散
| 特性 | |
|---|---|
| Ps,t | 0.2591 |
| PC,s | 0.5170 |
| Pd,C | 0.2999 |
| Pe,d | 0.2379 |
| Pg,F | 0.5590 |
| Pi,h | |
| P's,t | 0.2563 |
| P'C',s | 0.5585 |
| P'd,C' | 0.2498 |
| P'e,d | 0.2354 |
| P'g,F' | 0.4957 |
| P'i,h | |
| 特性 | |
|---|---|
| ΔPC,t | 0.0145 |
| ΔPC,s | 0.0077 |
| ΔPF,e | -0.0022 |
| ΔPg,F | -0.0080 |
| ΔPi,g | |
下载
TIE's - 技术信息
TIE-19: Temperature Coefficient of the Refractive Index (US)
PDF
450 kB
TIE-25: Striae in Optical Glass (US)
PDF
1.24 MB
TIE-27: Stress in Optical Glass (US)
PDF
710 kB
TIE-28: Bubbles and Inclusions in Optical Glass (US)
PDF
260 kB
TIE-29: Refractive Index and Dispersion (US)
PDF
1 MB
TIE-30: Chemical Properties of Optical Glass (US)
PDF
210 kB
TIE-31: Mechanical and Thermal Properties of Optical Glass (US)
PDF
220 kB
TIE-32: Thermal Loads on Optical Glass (US)
PDF
140 kB
TIE-33: Bending Strength of Optical Glass and ZERODUR® (US)
PDF
2.75 MB
TIE-35: Transmittance of Optical Glass (US)
PDF
500 kB
TIE-36: Fluorescence of Optical Glass (US)
PDF
1.02 MB
TIE-40: Optical Glass for Precision Molding (US)
PDF
610 kB
TIE-41: Large Optical Glass Blanks (US)
PDF
2.06 MB