BG45

承诺光谱值 | |
---|---|
τi (514nm) | ≥0.93 |
τi (700nm) | ≤0.001 |
- SCHOTT
- BG45 - BG45
- 厚度
- 1.0
- 反射系数
- 0.9110
λ [nm] | |
---|---|
200 | |
210 | |
220 | |
230 | |
240 | |
250 | |
260 | |
270 | |
280 | |
290 | |
300 | < 10⁻³ |
310 | 0.001 |
320 | 0.045 |
330 | 0.200 |
340 | 0.371 |
350 | 0.488 |
360 | 0.568 |
370 | 0.625 |
380 | 0.671 |
390 | 0.715 |
400 | 0.750 |
410 | 0.786 |
420 | 0.814 |
430 | 0.842 |
440 | 0.864 |
450 | 0.885 |
460 | 0.902 |
470 | 0.917 |
480 | 0.929 |
490 | 0.938 |
λ [nm] | |
---|---|
500 | 0.944 |
510 | 0.946 |
520 | 0.941 |
530 | 0.925 |
540 | 0.896 |
550 | 0.850 |
560 | 0.784 |
570 | 0.695 |
580 | 0.589 |
590 | 0.470 |
600 | 0.353 |
610 | 0.246 |
620 | 0.159 |
630 | 0.095 |
640 | 0.051 |
650 | 0.026 |
660 | 0.012 |
670 | 0.005 |
680 | 0.002 |
690 | < 10⁻³ |
700 | < 10⁻³ |
710 | < 10⁻³ |
720 | < 10⁻³ |
730 | < 10⁻³ |
740 | < 10⁻³ |
750 | < 10⁻³ |
760 | < 10⁻³ |
770 | < 10⁻³ |
780 | < 10⁻³ |
790 | < 10⁻³ |
λ [nm] | |
---|---|
800 | < 10⁻³ |
810 | < 10⁻³ |
820 | < 10⁻³ |
830 | < 10⁻³ |
840 | < 10⁻³ |
850 | < 10⁻³ |
860 | < 10⁻³ |
870 | < 10⁻³ |
880 | < 10⁻³ |
890 | < 10⁻³ |
900 | < 10⁻³ |
910 | < 10⁻³ |
920 | < 10⁻³ |
930 | < 10⁻³ |
940 | < 10⁻³ |
950 | < 10⁻³ |
960 | < 10⁻³ |
970 | < 10⁻³ |
980 | < 10⁻³ |
990 | < 10⁻³ |
1,000 | < 10⁻³ |
1,010 | < 10⁻³ |
1,020 | < 10⁻³ |
1,030 | < 10⁻³ |
1,040 | < 10⁻³ |
1,050 | < 10⁻³ |
1,060 | < 10⁻³ |
1,070 | < 10⁻³ |
1,080 | < 10⁻³ |
1,090 | < 10⁻³ |
λ [nm] | |
---|---|
1,100 | < 10⁻³ |
1,110 | < 10⁻³ |
1,120 | < 10⁻³ |
1,130 | < 10⁻³ |
1,140 | < 10⁻³ |
1,150 | < 10⁻³ |
1,160 | < 10⁻³ |
1,170 | < 10⁻³ |
1,180 | < 10⁻³ |
1,190 | < 10⁻³ |
1,200 | < 10⁻³ |
1,250 | < 10⁻³ |
1,300 | < 10⁻³ |
1,350 | 0.002 |
1,400 | 0.006 |
1,450 | 0.015 |
1,500 | 0.036 |
1,550 | 0.068 |
1,600 | 0.116 |
1,650 | 0.178 |
1,700 | 0.250 |
1,750 | 0.328 |
1,800 | 0.407 |
1,850 | 0.483 |
1,900 | 0.551 |
1,950 | 0.616 |
2,000 | 0.670 |
2,050 | 0.716 |
2,100 | 0.756 |
2,150 | 0.785 |
λ [nm] | |
---|---|
2,200 | 0.802 |
2,250 | 0.811 |
2,300 | 0.826 |
2,350 | 0.842 |
2,400 | 0.853 |
2,450 | 0.860 |
2,500 | 0.853 |
2,550 | 0.830 |
2,600 | 0.813 |
2,650 | 0.800 |
2,700 | 0.778 |
2,750 | 0.707 |
2,800 | 0.395 |
2,850 | 0.188 |
2,900 | 0.107 |
2,950 | 0.070 |
3,000 | 0.049 |
3,050 | 0.036 |
3,100 | 0.028 |
3,150 | 0.022 |
3,200 | 0.018 |
3,250 | 0.016 |
3,300 | 0.014 |
3,350 | 0.014 |
3,400 | 0.014 |
3,450 | 0.015 |
3,500 | 0.017 |
3,550 | 0.020 |
3,600 | 0.023 |
3,650 | 0.027 |
λ [nm] | |
---|---|
3,700 | 0.030 |
3,750 | 0.029 |
3,800 | 0.025 |
3,850 | 0.021 |
3,900 | 0.015 |
3,950 | 0.009 |
4,000 | 0.006 |
4,050 | 0.004 |
4,100 | 0.002 |
4,150 | 0.002 |
4,200 | 0.001 |
4,250 | 0.001 |
4,300 | 0.002 |
4,350 | 0.003 |
4,400 | 0.005 |
4,450 | 0.007 |
4,500 | 0.009 |
4,550 | 0.011 |
4,600 | 0.013 |
4,650 | 0.016 |
4,700 | 0.020 |
4,750 | 0.023 |
4,800 | 0.026 |
4,850 | 0.029 |
4,900 | 0.031 |
4,950 | 0.031 |
5,000 | 0.029 |
5,050 | 0.025 |
5,100 | 0.018 |
5,150 | 0.010 |
反射系数 | |
---|---|
Pd | 0.911 |
参考厚度 | |
---|---|
d [mm] | 1 |
承诺光谱值 | |
---|---|
τi (514nm) | ≥0.93 |
τi (700nm) | ≤0.001 |
折射率 n |
---|
nF (486.1 nm) = 1.557 |
nh (404.7 nm) = 1.569 |
ng (435.8 nm) = 1.563 |
ns (852.1 nm) = 1.543 |
ne (546.1 nm) = 1.552 |
nd (587.6 nm) = 1.550 |
色度评估
光源 | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.319 | 0.260 | 0.227 |
y | 0.445 | 0.453 | 0.455 |
Y | 55 | 41 | 33 |
λd [nm] | 500 | 499 | 499 |
Pe | 0.29 | 0.43 | 0.51 |
光源 | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.301 | 0.247 | 0.216 |
y | 0.426 | 0.430 | 0.429 |
Y | 56 | 43 | 35 |
λd [nm] | 498 | 497 | 497 |
Pe | 0.30 | 0.43 | 0.51 |
光源 | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.229 | 0.197 | 0.179 |
y | 0.324 | 0.318 | 0.315 |
Y | 63 | 51 | 43 |
λd [nm] | 491 | 490 | 490 |
Pe | 0.31 | 0.43 | 0.50 |
密度 | |
---|---|
p [g/cm3] | 2.7634 |
气泡含量 | |
---|---|
气泡等级 |
玻转温度 | |
---|---|
Tg [°C] | 384 |
温度系数 | |
---|---|
Tk [nm/°C] |
耐化学性 | |
---|---|
耐污性 | 0 |
耐酸性 | 4.0 |
耐碱性 | 4.3 |
热膨胀 | |
---|---|
α-30°C/+70°C [10-6/K] | 8.12 |
α20°C/300°C [10-6/K] | 10.09 |