FK5HTI
Glascode: 487705.245Um alle Funktionen des Shops nutzen zu können müssen Sie sich anmelden oder registriere dich
Technische Daten
Brechungsindizes
| Eigenschaften | λ [nm] | |
|---|---|---|
| n2.325,4 | 2.325,4 | 1,46180 |
| n1.970,1 | 1.970,1 | 1,46738 |
| n1.529,6 | 1.529,6 | 1,47312 |
| n1.060,0 | 1.060,0 | 1,47855 |
| nt | 1.014,0 | 1,47912 |
| ns | 852,1 | 1,48137 |
| nr | 706,5 | 1,48409 |
| nC | 656,3 | 1,48534 |
| nC' | 643,8 | 1,48568 |
| Eigenschaften | λ [nm] | |
|---|---|---|
| n632,8 | 632,8 | 1,48600 |
| nD | 589,3 | 1,48742 |
| nd | 587,6 | 1,48748 |
| ne | 546,1 | 1,48913 |
| nF | 486,1 | 1,49225 |
| nF' | 480,0 | 1,49264 |
| ng | 435,8 | 1,49591 |
| nh | 404,7 | 1,49892 |
| ni | 365,0 | 1,50398 |
| Eigenschaften | λ [nm] | |
|---|---|---|
| n334,1 | 334,1 | 1,50935 |
| n312,6 | 312,6 | 1,51423 |
| n296,7 | 296,7 | 1,51861 |
| n280,4 | 280,4 | 1,52409 |
| n248,3 | 248,3 | |
Reintransmissionsgrad
| Eigenschaften | λ [nm] | |
|---|---|---|
| τ25/2500 | 2.500 | 0,385 |
| τ25/2325 | 2.325 | 0,628 |
| τ25/1970 | 1.970 | 0,930 |
| τ25/1530 | 1.530 | 0,965 |
| τ25/1060 | 1.060 | 0,998 |
| τ25/700 | 700 | 0,997 |
| τ25/660 | 660 | 0,995 |
| τ25/620 | 620 | 0,994 |
| τ25/580 | 580 | 0,995 |
| τ25/546 | 546 | 0,995 |
| τ25/500 | 500 | 0,994 |
| τ25/460 | 460 | 0,995 |
| τ25/436 | 436 | 0,996 |
| τ25/420 | 420 | 0,997 |
| τ25/405 | 405 | 0,997 |
| τ25/400 | 400 | 0,997 |
| τ25/390 | 390 | 0,997 |
| τ25/380 | 380 | 0,996 |
| τ25/370 | 370 | 0,996 |
| τ25/365 | 365 | 0,996 |
| τ25/350 | 350 | 0,994 |
| τ25/334 | 334 | 0,989 |
| τ25/320 | 320 | 0,979 |
| τ25/310 | 310 | 0,958 |
| τ25/300 | 300 | 0,900 |
| τ25/290 | 290 | 0,760 |
| τ25/280 | 280 | 0,510 |
| τ25/270 | 270 | 0,220 |
| τ25/260 | 260 | 0,050 |
| τ25/250 | 250 | 0,002 |
| Eigenschaften | λ [nm] | |
|---|---|---|
| τ10/2500 | 2.500 | 0,683 |
| τ10/2325 | 2.325 | 0,830 |
| τ10/1970 | 1.970 | 0,971 |
| τ10/1530 | 1.530 | 0,986 |
| τ10/1060 | 1.060 | 0,999 |
| τ10/700 | 700 | 0,999 |
| τ10/660 | 660 | 0,998 |
| τ10/620 | 620 | 0,998 |
| τ10/580 | 580 | 0,998 |
| τ10/546 | 546 | 0,998 |
| τ10/500 | 500 | 0,998 |
| τ10/460 | 460 | 0,998 |
| τ10/436 | 436 | 0,998 |
| τ10/420 | 420 | 0,999 |
| τ10/405 | 405 | 0,999 |
| τ10/400 | 400 | 0,999 |
| τ10/390 | 390 | 0,999 |
| τ10/380 | 380 | 0,998 |
| τ10/370 | 370 | 0,999 |
| τ10/365 | 365 | 0,998 |
| τ10/350 | 350 | 0,998 |
| τ10/334 | 334 | 0,996 |
| τ10/320 | 320 | 0,992 |
| τ10/310 | 310 | 0,983 |
| τ10/300 | 300 | 0,959 |
| τ10/290 | 290 | 0,896 |
| τ10/280 | 280 | 0,764 |
| τ10/270 | 270 | 0,546 |
| τ10/260 | 260 | 0,302 |
| τ10/250 | 250 | 0,120 |
Teildispersion
| Eigenschaften | |
|---|---|
| Ps,t | 0,3253 |
| PC,s | 0,5742 |
| Pd,C | 0,3098 |
| Pe,d | 0,2388 |
| Pg,F | 0,5288 |
| Pi,h | 0,7315 |
| P's,t | 0,3234 |
| P'C',s | 0,6203 |
| P'd,C' | 0,2584 |
| P'e,d | 0,2374 |
| P'g,F' | 0,4703 |
| P'i,h | 0,7271 |
| Eigenschaften | |
|---|---|
| ΔPC,t | 0,0202 |
| ΔPC,s | 0,0070 |
| ΔPF,e | 0,0001 |
| ΔPg,F | 0,0036 |
| ΔPi,g | 0,0321 |
Downloads
Datenblatt
Datenblatt-Sammlung
TIE‘s - Technische Informationen
TIE-19: Temperature Coefficient of the Refractive Index (US)
PDF
450 kB
TIE-25: Striae in Optical Glass (US)
PDF
1,24 MB
TIE-27: Stress in Optical Glass (US)
PDF
710 kB
TIE-28: Bubbles and Inclusions in Optical Glass (US)
PDF
260 kB
TIE-29: Refractive Index and Dispersion (US)
PDF
1 MB
TIE-30: Chemical Properties of Optical Glass (US)
PDF
210 kB
TIE-31: Mechanical and Thermal Properties of Optical Glass (US)
PDF
220 kB
TIE-32: Thermal Loads on Optical Glass (US)
PDF
140 kB
TIE-33: Bending Strength of Optical Glass and ZERODUR® (US)
PDF
2,75 MB
TIE-35: Transmittance of Optical Glass (US)
PDF
500 kB
TIE-36: Fluorescence of Optical Glass (US)
PDF
1,02 MB
TIE-40: Optical Glass for Precision Molding (US)
PDF
610 kB
TIE-41: Large Optical Glass Blanks (US)
PDF
2,06 MB