F2G12 621366.360

肖特先进光学事业部提供具有不同色散特性 的多种耐辐射玻璃类型。这些玻璃类型非常 适合在具有高辐射性的环境中使用。
特性 | |||
---|---|---|---|
nd | 1.62072 | νd | 36.56 |
ne | 1.62474 | νe | 36.30 |
nF-nC | 0.016979 | nF'-nC' | 0.017212 |
特性 | λ [nm] | |
---|---|---|
n2,325.4 | 2,325.4 | 1.58584 |
n1,970.1 | 1,970.1 | 1.59051 |
n1,529.6 | 1,529.6 | 1.59593 |
n1,060.0 | 1,060.0 | 1.60265 |
nt | 1,014.0 | 1.60353 |
ns | 852.1 | 1.60744 |
nr | 706.5 | 1.61298 |
nC | 656.3 | 1.61573 |
nC' | 643.8 | 1.61652 |
特性 | λ [nm] | |
---|---|---|
n632.8 | 632.8 | 1.61725 |
nD | 589.3 | 1.62057 |
nd | 587.6 | 1.62072 |
ne | 546.1 | 1.62474 |
nF | 486.1 | 1.63271 |
nF' | 480.0 | 1.63373 |
ng | 435.8 | 1.64261 |
nh | 404.7 | 1.65121 |
ni | 365.0 |
特性 | λ [nm] | |
---|---|---|
n334.1 | 334.1 | |
n312.6 | 312.6 | |
n296.7 | 296.7 | |
n280.4 | 280.4 | |
n248.3 | 248.3 |
特性 | λ [nm] | |
---|---|---|
τ25/2500 | 2,500 | 0.750 |
τ25/2325 | 2,325 | 0.820 |
τ25/1970 | 1,970 | 0.930 |
τ25/1530 | 1,530 | 0.989 |
τ25/1060 | 1,060 | 0.997 |
τ25/700 | 700 | 0.988 |
τ25/660 | 660 | 0.984 |
τ25/620 | 620 | 0.979 |
τ25/580 | 580 | 0.972 |
τ25/546 | 546 | 0.963 |
τ25/500 | 500 | 0.937 |
τ25/460 | 460 | 0.850 |
τ25/436 | 436 | 0.650 |
τ25/420 | 420 | 0.400 |
τ25/405 | 405 | 0.120 |
τ25/400 | 400 | 0.060 |
τ25/390 | 390 | 0.000 |
τ25/380 | 380 | |
τ25/370 | 370 | |
τ25/365 | 365 | |
τ25/350 | 350 | |
τ25/334 | 334 | |
τ25/320 | 320 | |
τ25/310 | 310 | |
τ25/300 | 300 | |
τ25/290 | 290 | |
τ25/280 | 280 | |
τ25/270 | 270 | |
τ25/260 | 260 | |
τ25/250 | 250 |
特性 | λ [nm] | |
---|---|---|
τ10/2500 | 2,500 | 0.891 |
τ10/2325 | 2,325 | 0.924 |
τ10/1970 | 1,970 | 0.971 |
τ10/1530 | 1,530 | 0.996 |
τ10/1060 | 1,060 | 0.999 |
τ10/700 | 700 | 0.995 |
τ10/660 | 660 | 0.994 |
τ10/620 | 620 | 0.992 |
τ10/580 | 580 | 0.989 |
τ10/546 | 546 | 0.985 |
τ10/500 | 500 | 0.974 |
τ10/460 | 460 | 0.937 |
τ10/436 | 436 | 0.842 |
τ10/420 | 420 | 0.693 |
τ10/405 | 405 | 0.428 |
τ10/400 | 400 | 0.325 |
τ10/390 | 390 | 0.124 |
τ10/380 | 380 | 0.019 |
τ10/370 | 370 | 0.000 |
τ10/365 | 365 | |
τ10/350 | 350 | |
τ10/334 | 334 | |
τ10/320 | 320 | |
τ10/310 | 310 | |
τ10/300 | 300 | |
τ10/290 | 290 | |
τ10/280 | 280 | |
τ10/270 | 270 | |
τ10/260 | 260 | |
τ10/250 | 250 |
特性 | |
---|---|
Ps,t | 0.2303 |
PC,s | 0.4883 |
Pd,C | 0.2937 |
Pe,d | 0.2369 |
Pg,F | 0.5831 |
Pi,h | |
P's,t | 0.2272 |
P'C',s | 0.5271 |
P'd,C' | 0.2443 |
P'e,d | 0.2337 |
P'g,F' | 0.5163 |
P'i,h |
特性 | |
---|---|
ΔPC,t | 0.0002 |
ΔPC,s | 0.0002 |
ΔPF,e | 0.0002 |
ΔPg,F | 0.0008 |
ΔPi,g |
TIE‘s - Technical Information
- TIE-04: Test Report for Delivery Lots of Optical Glass-May 2016
- TIE-19: Temperature coefficient of Refractive Index-July 2016
- TIE-25: Striae in Optical Glass-June 2006
- TIE-26: Homogeneity of Optical Glass-February 2016
- TIE-27: Stress in Optical Glass-July 2004
- TIE-28: Bubbles and Inclusions in Optical Glass-May 2016
- TIE-29: Refractive Index and Dispersion-February 2016
- TIE-30: Chemical properties of Optical Glass-February 2016
- TIE-31: Mechanical and Thermal Properties of Optical Glass-July 2004
- TIE-32: Thermal Loads on Optical Glass-August 2004
- TIE-33: Bending Strength of Optical Glass and ZERODUR®-December 2015
- TIE-35: Transmittance of Optical Glass-October 2005
- TIE-36: Fluorescence of Optical Glass-August 2010
- TIE-40: Optical Glass for Precision Molding-September 2011
- TIE-41: Large Optical Glass Blanks-September 2006
- TIE-42: Radiation Resistant Optical Glasses-April 2018